EU Norms (EN 459) Mandatory testing program

for Natural Hydraulic Limes

POWDERS
TEST
NORM
EN459 Values
St Astier Values
Frequency
St.Astier Frequency
Fineness
EN196-6
residue by mass 0.09mm/0.2mm <15%/<5%
5-7%
daily
daily
Free water
EN459-2
NHL2/3.5<2
<2
NHL5<1
<1
monthly
monthly
Soundness (Expansion)
EN459-2
<2
<1
once a day
several times per day
Bulk density Kg/dm3
EN459-2
NHL20.4-0.8
0.56
monthly
each product batch
NHL3.50.5-0.9
0.61/0.65
NHL50.6-1.0
0.66/0.75
MORTARS (prepared with standard EU sand/ISO 679 @ 1:1 vol. ratio
Penetration
EN459-2
>20mm
>20mm
monthly
weekly
<50mm
<50mm
Setting time
EN459-2
>1h/<15h
>3h/<10h
2 per week
2 per week
Air content
EN459-2
<20
<20
monthly
monthly
Compressive
EN459-2
28 days
weekly
continuously
Srength
N/mm2
NHL2
2 to 7
2 to 3
NHL3.5
3.5 to 10
3.5 to 6
NHL5
5 to 15
5 to 9
SO3
EN196-2
content %
3*
0.45/0.65
monthly
continuously
*up to 7% admissible if soundness is demonstrated at 28 days of water curing
Available
EN459-2
NHL53%
15-20%
weekly
each product batch
Lime
minimum
NHL3.59%
22-26%
each product batch
values
NHL215%
50-55%
each product batch

Other tests regularly performed by the Saint-Astier® Research & Development Dept: CO2 contents after each burning to regulate slaking, tensile strength, elasticity moduli, adhesion, workability (flow table), whiteness.